The Structural Properties of $Bi_4Ti_3O_{12}$ Ferroelectric Thin Films doped with Cerium

Cerium이 첨가된 $Bi_4Ti_3O_{12}$ 강유전체 박막의 구조적 특성

  • Published : 2005.11.10

Abstract

The structural properties of $(Bi,Ce)_4Ti_3O_{12}(BCT)$ thin films with post-annealing temperature were investigated. $(Bi,Ce)_4Ti_3O_{12}(BCT)$ thin films were deposited by RF sputtering method on Pt/Ti/$SiO_2$/Si substrates with optimum deposition condition. The $(Bi,Ce)_4Ti_3O_{12}(BCT)$ thin films was post-annealed at 600$^{\circ}C$, 650$^{\circ}C$, 700$^{\circ}C$, 750$^{\circ}C$, 800$^{\circ}C$ in furnace,respectively. Increasing the post-annealing temperature, the grain size, density and peak intensity of (117) and c-axis orientation were increased. The $(Bi,Ce)_4Ti_3O_{12}(BCT)$ thin films that annealed at 750$^{\circ}C$ exhibited well crystallized phase and had no vacancy and grain was uniform. but there are some secondary phases observed. At this time, the average thickness of $(Bi,Ce)_4Ti_3O_{12}(BCT)$ thin films was 2000 ${\AA}$.

Keywords