A Study on the Characteristics of Mine Liner According to the Contents of CSA Using Industrial Byproducts

산업부산물을 활용한 CSA 첨가량에 따른 광산 차수재 특성에 관한 연구

  • Received : 2019.02.25
  • Accepted : 2019.03.12
  • Published : 2019.03.30

Abstract

In this study, to characterize the application of CSA and dihydrate gypsum Utilizing industrial byproducts, we investigated the characteristics of CSA and dihydrate gypsum to investigate the characteristics of Mine Liner according to the addition amount. As a result of compressive strength, length change and absorption rate of mining lime wastewater according to CSA addition amount, up to 30% of CSA showed a positive effect on shrinkage and absorption reduction effect as well as strength at initial age. However, due to excessive use of CSA 50%, it was reduced by 15% compared to OPC due to increase of absorption rate and decrease of cement amount due to over expansion rather than shrinkage compensation and void filling.

본 연구에서는 산업부산물을 활용한 CSA와 이수석고를 광산 차수재에 적용하기 위한 기초자료를 제시하고자 CSA와 이수석고 첨가량에 따른 차수재의 특성을 검토하였으며 그 결과를 다음과 같이 나타내었다. CSA 첨가량에 따른 광산 차수재의 압축강도, 길이변화, 흡수율 측정결과 CSA30%까지는 초기재령에서의 강도증가와 더불어 수축 및 흡수율저감 효과에 긍정적인 영향을 미치는 것으로 나타났다. 그러나 CSA50%에서는 과량 사용으로 인하여 수축보상 및 공극충진보다는 과팽창으로 인한 흡수율 증가와 시멘트양 감소로 인하여 OPC와 비교하여 15% 감소하였다.

Keywords

GSJHDK_2019_v7n1_74_f0001.png 이미지

Fig. 1. Demec strain gauge

GSJHDK_2019_v7n1_74_f0002.png 이미지

Fig. 2. Flow according to the CSA contents

GSJHDK_2019_v7n1_74_f0003.png 이미지

Fig. 3. Compressive strength according to the CSA contents

GSJHDK_2019_v7n1_74_f0004.png 이미지

Fig. 4. Compressive strength ratio according to the CSA contents

GSJHDK_2019_v7n1_74_f0005.png 이미지

Fig. 5. Rate of length change

GSJHDK_2019_v7n1_74_f0006.png 이미지

Fig. 6. Absorption ratio

GSJHDK_2019_v7n1_74_f0007.png 이미지

Fig. 7. Incremental void distribution volume

GSJHDK_2019_v7n1_74_f0008.png 이미지

Fig. 8. Cumulative void volume

Table 1. Experiment plan and mix design

GSJHDK_2019_v7n1_74_t0001.png 이미지

Table 4. Chemical compositions of raw Materials

GSJHDK_2019_v7n1_74_t0002.png 이미지

Table 2. Physical properties and chemical composition of OPC and slag

GSJHDK_2019_v7n1_74_t0003.png 이미지

Table 3. Physical properties and chemical composition of drystalline gypsum

GSJHDK_2019_v7n1_74_t0004.png 이미지

References

  1. Kim, M.G., Kim, K.J., Jeong, G.C. (2018). Assessment of the cause and pathway of contamination and sustainability in an abandoned mine, The Journal of Engineering Geology, 28(3), 411-429 [in Korean]. https://doi.org/10.9720/kseg.2018.3.411
  2. Lee, S.E., Park, S.J., Kim, H.S., Jang, H.S., Kim, T.H. (2012). A study on the model test for mine filling using coal ash, Tunnel and Underground Space, 22(6), 449-461 [in Korean]. https://doi.org/10.7474/TUS.2012.22.6.449
  3. Kim, T.W., Hahm, H.G. (2012). Mechanical properties of the alkaliactivated slag mortar with gypsum, Journal of The Korea Institute for Structural Maintenance and Inspection, 16(3), 109-116 [in Korean]. https://doi.org/10.11112/jksmi.2012.16.3.109
  4. Sakai, E., Raina, K., Asaga, K., Goto, S., Kondo, R. (1980). Influence of sodium aromatic sulfonates on the hydration of tricalcium aluminate with or without gypsym, Cement and Concrete Research, 10(3), 311-319. https://doi.org/10.1016/0008-8846(80)90107-6
  5. Lee, H.W., Min, S.E., Lee, K.H., Kim, C.S., Eom, H.J. (2014). Characterization of high early strength type shrinkage reducing cement utilizing CSA expansion admixture of low-activity, Journal of Korean Recycled Construction Resources Institute, 9(2), 38-45 [in Korean].
  6. Kim, Y.U., Kim, D.B., Choi, S.J. (2018). An experimental study on the setting time and compressive strength of mortar using ferronickel slag powder, Journal of the Korea Institute of Building Construction, 18(6), 551-558 [in Korean]. https://doi.org/10.5345/JKIBC.2018.18.6.551
  7. Han, C.G., Lee, M.H., Park, Y.S., Pei, C.C. (2005). Physical properties of concrete with the contents of CSA expansive admixture, Magazine of the Korea Concrete Institute, 5, 369-372 [in Korean].
  8. Park, C.B., Ryu, D.H., Seo, C.H. (2012). Properties of high volume mineral admixtures concrete using inorganic additives, Journal of the Architectural Institute of Korea, 28(3), 631-637 [in Korean].
  9. Sung, C.J., Song, M.S., Lee, K.H., Han, C.G. (2002). Hydration of expansive materials with CSA-system, Journal of the Korea Concrete Institute, 14(5), 631-637 [in Korean]. https://doi.org/10.4334/JKCI.2002.14.5.631
  10. Cho, Y.K., Nam, S.Y., Kim, C.S., Lee, H.W., Jo, S.H., Ahn, J.W. (2018). Evaluation of physical properties of mine polymer liner and cover material containing re-emulsification type EVA resin, The Polymer Society Of Korea, 42(4), 637-642 [in Korean]. https://doi.org/10.7317/pk.2018.42.4.637
  11. Joo, M.K., Lho, B.C. (2015). Evaluation of properties of polymer-modified mortar with CSA, Journal of the Korea Institute for Structural Maintenance and Inspection, 19(1), 35-44 [in Korean]. https://doi.org/10.11112/jksmi.2015.19.1.035
  12. Song, H.S., Lee, C.Y., Min, C.S. (2007). Hydration of high volume mineral admixtures binder with kind of activators, Journal of the Korea Institute for Structural Maintenance Inspection, 11(1), 85-94 [in Korean].