Introduction
In recent years, self-assembled monolayers (SAMs) have provoked intense interest due to their nanometer size, highly- ordered structures and ion recognition properties.1,2 Organosulfur compounds and their derivatives are particularly attractive due to their ease of preparation and the spontaneous adsorption and organization of them on the gold electrode surfaces to form the extraordinary ordered monolayers through self-assembling.3-6 A number of applications for such SAMs have been explored, including nanolithography and chemical sensors.7-9 Notably, SAMs have been employed in organic electronic devices to modify the work function of the electrodes.10-14
Self-assembled monolayers (SAMs) are formed at a solidliquid interface by molecules consisted of three units: a headgroup that binds to the substrate, a tailgroup that constitutes the outer surface of the film, and a backbone, usually a long chain, that connects the headgroup and the tailgroup. While pure alkylthiols are known to form SAMs that exhibit order on a large scale,15-18 π-conjugated thiols and their derivatives seem to be a better choice for applications in organic- and single-molecule electronics because of their intrinsic semiconducting properties. Relatively recently, Piotrowski et al.19 reported the synthesis and electronic properties of thioacetate-functionalized fullerene, Park et al.20 studied the formation of octylthioacetates SAMs on gold in the vapor phase. Moreover the monolayer films based on aromatic sulfur compounds offer an opportunity to enhance the electrical coupling between the electronic states of the electrode and the redox species in solution.
Scheme 1
Herein, we design two classes of morpholino-substitued thioacetate, and the different barrier property of the monolayer films formed on Au electrode is studied by using electrochemical techniques. The ion recognition properties of self-assembled monolayers using cyclic voltammetry are studied. We find that the arenethioacetate forms higherquality close-packed organic layers than alkanethioacetate and both of them have an apparent and fast capacity in recognition for Ag+.
Experimental
Materials. Synthesis and characterization of S-(3-morpho-linopropyl) ethanethioate (1), 2-(4-(3-morpholinopropoxy)-phenoxy) ethyl methanesulfonate (2)21 and S-(2-(4-(3-morpholinopropoxy)phenoxy)ethyl)ethanethioate (3) (Scheme 1) had been described elsewhere in detail.22 All chemicals were analytical grade and used without further purification.
Preparation of Substrates. The gold disk electrode (CHI, 2 mm in diameter) was pretreated using the following procedure prior to monolayer deposition. The electrode was cleaned in piranha solution, which is a mixture of 30% H2O2 and concentrated H2SO4 in 1:3 ratios. Then it was polished with alumina powder (diameter, 0.3 and 0.05 μm) followed by sonication in ethanol and deionized water. After copious rinsing with deionized water, the electrode was electrochemically cleaned by cycling the potential from 0.5 to 1.6 V at 50 mV s˗1 in 0.5 M sulfuric acid until typical cyclic voltammogram of clean gold was obtained.23,24
Preparation of SAMs and Mixed SAMs. The pretreated gold electrodes were immersed in 10 mM 1 and 3 acetone solution for about 24 h at ambient temperature (25 ± 1 ℃) respectively. Then the modified electrodes were removed from the solution and rinsed with deionized water, and dried with high purity nitrogen. The SAMs-modified gold electrodes were obtained and used for the electrochemical measurements immediately.
We had further tried to improve the blocking ability by forming a mixed SAMs with decanethiol. Immediately after the adsorption of corresponding compounds, the monolayer coated electrodes were rinsed with deionized water and dipped in 10 mM decanethiol-methanol solution for mixed SAMs formation. After 10 h at ambient temperature, the mixed SAMs modified electrodes were rinsed with deionized water and dried with high purity nitrogen, and subsequently analyzed using electrochemical studies.
Electrochemical Measurements. Electrochemical measurements were conducted by a PC controlled CHI920C electrochemical workstation bipotentiostat (CHI, Shanghai Chenhua Co.). A conventional three-electrode electrochemical cell with a Pt wire as a counter electrode, a Ag/AgCl (3 M KCl) electrode as a reference electrode and SAM-modified Au electrode as working electrode was used for the electrochemical characterization of SAMs.
Cyclic voltammetry (CV) measurements were operated in 5 mM K3[Fe(CN)6] with 0.1 M KCl at a potential range of ˗0.2 to 0.5 V. The impedance measurements were carried out using an ac signal of 10 mV amplitude at a formal potential of the redox couple at a wide frequency range of 100 kHz to 0.1 Hz. From the impedance data, the charge transfer resistance (Rct) was determined using the equivalent circuit fitting analysis. The impedance spectroscopy data were used for the equivalent circuit fitting analysis using ZSimpwin software.
Results and Discussion
Cyclic Voltammetry. Figure 1 showed the cyclic voltammograms of bare Au and SAMs-modified electrodes in 5 mM [Fe(CN)6]3˗/4˗ with 0.1 M KCl at a potential scan rate of 50mV s˗1. As it could be seen from Figure 1A(a), for the bare Au electrode, the reversible characteristic peak for the redox couple was observed, indicating that the electron transfer reaction was completely diffusion controlled. However, for the 1/Au and 3/Au electrodes (Figure 1A(b, c)), it was clearly seen that a significantly blocking behavior could be found. For the 1/C10SH/Au and 3/C10SH/Au electrodes (Figure 1B), no typical peak of the redox couple was observed. This might be ascribed to the fact that compound 1 (or 3) and C10SH anchored on the surface of Au electrode assembled a highly ordered, compact monolayer which completely inhibited the redox reaction. It could also be observed that in the case of compound 3 (Figure 1A(c), Figure 1B(b)), the CVs exhibited a rather better blocking behavior, which indicated the compound structure had an effect on the form of SAMs. The arenethioacetate SAMs was dominated by the π-π interactions between the benzene rings, while the alkanethioacetate SAMs was driven by the van der Waals interactions between the CH2 groups. Therefore arenethioacetate could form high-quality close-packed organic layers and had a bigger barrier for charge-carrier injection at the electrode-liquid interface.
Figure 1.(A) Cyclic voltammograms of Au (a), 1/Au (b), 3/Au (c) in 5.0 mmol/L K3[Fe(CN)6]/0.1 mol/L KCl. (B) Cyclic voltammograms of 1/C10SH/Au (a), 3/C10SH/Au (b) in 5.0 mmol/L K3[Fe(CN)6]/0.1 mol/L KCl. Scan rate: 50 mV s˗1.
Figure 2 showed the cyclic voltammograms of SAMs-modified electrodes in 5 mM [Fe(CN)6]3˗/4˗ at different scan rates. The corresponding insets of these Figures showed that the reductive peak current (Ipc) had a direct linear relationship with the square root of scan rate. The linear regression equations were Ipc = 2.2205 v1/2 + 10.4728 (R = 0.9974), Ipc = 3.3552 v1/2 + 2.3873 (R = 0.9999), respectively, which meant the electron transfer process was essentially diffusion controlled.
Figure 2.Cyclic voltammograms of 1/Au (a), 3/Au (b), 1/C10SH/ Au (c), 3/C10SH/Au (d) in 5.0 mmol/L K3[Fe(CN)6] /0.1 mol/L KCl. Scan rate (from a to h): 25, 50, 75, 100, 125, 150, 175, 200 mV s˗1. Inset: Ipc-v1/2.
Figure 3.Impedance plots of Au, 1/Au, 3/Au, 1/C10SH/Au, 3/ C10SH/Au in 5.0 mmol/L K3[Fe(CN)6]/0.1 mol/L KCl.
Electrochemical Impedance Spectroscopy. Figure 3 showed the Nyquist plots of bare Au and SAMs-modified gold electrodes in 5 mM [Fe(CN)6]3˗/4˗ with 0.1 M KCl. It could be seen from the Figure 3 that the bare Au electrode showed a low frequency straight line with a very small semicircle at high frequency region indicating that the electron transfer process was essentially diffusion-controlled. For the SAM or mixed SAMs modified electrodes, it could be seen that large semicircles at the high frequency region of impedance plots were observed, implying a good blocking behavior for the redox reaction. It could also be noted from Figure 3 that the impedance values were much higher in the case of SAM of compound 3, which indicated a better blocking ability of the SAM towards the redox reaction. The results were in conformity with our studies using cyclic voltammetry.
According to the data obtained from the Nyquist plots, the value of R0 and Rct could be calculated (where R0 was the charge transfer resistance of bare Au electrode and Rct was the charge transfer resistance of the corresponding different SAM-modified electrodes). Rct was a measure of blocking ability of the monolayer films towards the electron transfer reaction. Higher the Rct values better the blocking behaviour of monolayers. Table 1 showed some measured parameters of bare gold and SAM-modified electrodes obtained from the impedance plots. From the table the charge transfer resistance values, we could calculate the surface coverage (θ) of the monolayer on the gold electrode using equation θ = 1 ˗ (R0/Rct), by assuming that the current was attributed to the presence of pinholes and defects within the monolayer.25,26 From the calculated Rct and surface coverage values, it was clear that the blocking ability of these SAMs followed the order 3/Au > 1/Au.
Table 1.The charge transfer resistance (Rct) and the surface coverage (θ) of compound 1 and 3 on the gold surface
Figure 4.(A) Ag+ at the SAMs of 1 (a), 3 (b) on Au electrode in 0.1 mol/L KCl; (B) Cu2+ at the SAMs of 1 (a), 3 (b) on Au electrode in 0.1 mol/L KCl; (C) Pb2+ at the SAMs of 1 (a), 3 (b) on Au electrode in 0.1 mol/L KCl; (D) Fe3+ at the SAMs of 1 (a), 3 (b) on Au electrode in 0.1 mol/L KCl. Scan rate: 50 mV s˗1.
Ion Recognition. Ag+, Cu2+, Pb2+ and Fe3+, carrying different charges, were used to investigate the electrochemical properties of the 1/Au and 3/Au electrode. Immediately prior to use, the SAMs-modified Au electrodes were immersed in a freshly prepared 5 mM aqueous solution of silver nitrate, copper sulfate, lead acetate and iron trichloride for 8 h followed by rinsing with deionized water. It could be seen from Figure 4(A) that the 1/Au and 3/Au electrode enriched of Ag+ showed reversible redox peaks indicating that Ag+ was adsorbed to the SAMs. In contrast, the absence of any peak formation in the CVs of Cu2+, Pb2+ and Fe3+ at the 1/Au and 3/Au electrodes (Figure 4(B), Figure 4(C), Figure 4(D)) indicated that they could not be adsorbed to the SAMs.
Figure 5.Cyclic voltammograms of 1/Au (A), 3/Au (B), 1/C10SH/Au (C), 3/C10SH/Au (D) electrode adsorbed Ag+ in 0.1 mol/L KCl. Deposition time (from a to g): 10 s, 30 s, 60 s, 5 min, 30 min, 60 min, 4 h. Inset: deposition time at 10 s.
Figure 6.(a) SEM image and EDS spectrum of 1-silver modified electrode, (b) SEM image and EDS spectrum of 3-silver modified electrode.
We had further studied the recognition speed of Ag+ on SAM-modified electrode. It could be seen from Figure 5 (inset), when the deposition time was 10 s, it showed a reversible redox peak. With the increase of deposition time, the current increased, which meant that more silver ions were adsorbed to the SAMs-modified electrode.
Furthermore, SEM, along with EDS measurements provide additional evidence about the recognition for Ag+. Figure 6(a, b) showed the SEM and EDS analysis of SAMs of 1-silver and 3-silver. The Ag composition of them was 2.9% and 4.34% respectively.
Conclusion
In this study, two different classes of thioacetate were synthesized: one class contained a alkyl chain, the other had a phenoxy backbone. Electrochemical techniques such as cyclic voltammetry and electrochemical impedance spectroscopy were employed to evaluate the barrier property of monolayer films using potassium ferro/ferri cyanide redox couple as a probe. We found from our results that the arenethioacetate formed high-quality close-packed organic layers. The electron transfer reaction of [Fe(CN)6]3˗/4˗ was completely inhibited on the mixed SAMs modified surfaces. From the cyclic voltammograms of SAMs-modified electrodes, all of them had an apparent and fast capacity in recognition for Ag+. SEM and EDS measurements had been used to prove it.
참고문헌
- Love, J. C.; Estroff, L. A.; Kriebel, J. K.; Nuzzo, R. G.; Whitesides, G. M. Chem. Rev. 2005, 105, 1103. https://doi.org/10.1021/cr0300789
- Zhang, S.; Cardona, C. M.; Echegoyen, L. Chem. Commun. 2006, 4461.
- Stouffer, J. M.; McCarthy, T. J. Macromolecules 1988, 21, 1204. https://doi.org/10.1021/ma00183a003
- Burshtain, D.; Mandler, D. J. Electroanal. Chem. 2005, 581, 310. https://doi.org/10.1016/j.jelechem.2005.05.006
- Holmlin, R. E.; Chen, X. X.; Chapman, R. G.; Takayama, S.; Whitesides, G. M. Langmuir 2001, 17, 2841. https://doi.org/10.1021/la0015258
- Li, Z. G.; Niu, T. X.; Zhang, Z. J.; Feng, G. Y.; Bi, S. P. J. Analyst. 2012, 137, 1680. https://doi.org/10.1039/c2an15716k
- Eck, W.; Stadler, V.; Geyer, W.; Zharnikov, M.; Golzhauser, A.; Grunze, M. Adv. Mater. 2000, 12, 805. https://doi.org/10.1002/(SICI)1521-4095(200006)12:11<805::AID-ADMA805>3.0.CO;2-0
- Felgenhauer, T.; Yan, C.; Geyer, W.; Rong, H. T.; Golzhauser, A.; Buck, M. Appl. Phys. Lett. 2001, 79, 3323. https://doi.org/10.1063/1.1415771
- Hobara, D.; Imabayashi, S.; Kakiuchi, T. Nano. Lett. 2002, 2, 1021. https://doi.org/10.1021/nl0256863
- Zhang, Y.; Salaita, K.; Lim, J. H.; Mirkin, C. A. Nano. Lett. 2002, 2, 1389. https://doi.org/10.1021/nl0202298
- Zehner, R. W.; Parsons, B. F.; Hsung, R. P.; Sita, L. R. Langmuir. 1999, 15, 1121. https://doi.org/10.1021/la981114f
- Alloway, D. M.; Hofmann, M.; Smith, D. L.; Gruhn, N. E.; Graham, A. L.; Colorado, R. J.; Wysocki, V. H.; Lee, T. R.; Lee, P. A.; Armstrong, N. R. J. Phys. Chem. B 2003, 107, 11690. https://doi.org/10.1021/jp034665+
- Campbell, I. H.; Rubin, S.; Zawodzinski, T. A. J. P. Phys. Rev. B 1996, 54, 14321. https://doi.org/10.1103/PhysRevB.54.R14321
- Shon, Y. S.; Lee, T. R. J. Phys. Chem. B 2000, 104, 8192. https://doi.org/10.1021/jp000651h
- Yang, Y. T.; Jamison, A. C.; Barriet, D.; Lee, T. R.; Ruths, M. J. Adhes. Sci. Technol. 2010, 24, 2511. https://doi.org/10.1163/016942410X508253
- Ma, F.; Lennox, R. B. Langmuir 2000, 16, 6188. https://doi.org/10.1021/la9913046
- Yokota, Y.; Fukui, K. I.; Enoki, T.; Hara, M. J. Phys. Chem. C 2007, 111, 7561. https://doi.org/10.1021/jp072249+
- Lee, L. Y. S.; Lennox, R. B. Langmuir 2007, 23, 292. https://doi.org/10.1021/la061684c
- Piotrowski, P.; Pawlowska, J.; Palys, B.; Sek, S.; Bilewicz, R.; Kaim, A. J. Electrochem. Soc. 2013, 160, H28.
- Park, T.; Kang, H.; Kim, Y.; Lee, S.; Noh, J. Bull. Korean Chem. Soc. 2011, 32, 39. https://doi.org/10.5012/bkcs.2011.32.1.39
- Sun, Y. Q.; Xi, H. T.; Chen, Y.; Sun, X. Q.; Chin. J. Syn. Chem. 2013, 21, 200.
- Sanders, W.; Vargas, R.; Anderson, M. R. Langmuir 2008, 24, 6133. https://doi.org/10.1021/la704059q
- Xi, H. T.; Ju, S. L.; Chen, Z. D.; Sun, X. Q. Chem. Lett. 2010, 39, 415. https://doi.org/10.1246/cl.2010.415
- Finklea, H. O.; Snider, D. A.; Fedyk, J.; Sabatani, E.; Gafni, Y.; Rubinstein, I. Langmuir 1993, 9, 3660. https://doi.org/10.1021/la00036a050
- Protsailo, L. V.; Fawcett, W. R. Langmuir 2002, 18, 8933. https://doi.org/10.1021/la0201218
피인용 문헌
- Phthalocyanine Monolayers Self-Assembled Directly from its Thiobenzoyl Derivative vol.9, pp.5, 2020, https://doi.org/10.1149/2162-8777/ab9a5e