Abstract
To analyze the phenomenon of corrosion in the PV module, we experimented damp heat test at $85^{\circ}C$/85% relative humidity(RH) and $65^{\circ}C$/85% RH for 2,000 hours, respectively. We used 30 mini-modules designed of 6inch one cell. Despite of 2,000 hours test, measured $P_{max}$ is not reached failure which is defined less than 80% compared to initial $P_{max}$. Therefore, we calculate proper curve fitting over 2,000 hours. Data less than 80% $P_{max}$ is found and B10 lifetime is calculated by the number of failure specimens and weibull distribution. Using B10 lifetime that the point of failure rate 10% and Peck's model, the predictable equation of lifetime was derived under temperature and humidity condition.