착화합물로써 EDTA이 사용된 $Gd_{2}O_{3}:Eu^{3+}$ 형광체의 합성 및 발광 특성

Synthesis and luminescent properties of $Gd_{2}O_{3}:Eu^{3+}$ red phosphors used EDTA

  • 발행 : 2003.04.19

초록

The synthesis and luminescent properties of trivalent europium activated gadolinium oxide red phosphors by sol-gel process have been investigated. Aqueous metal nitrate solution was mixed with EDTA which was chosen by the most suitable material of sol-gel formation as chelating agents. We noticed that the samples when are heated with EDTA at a temperature of $100^{\circ}C$ for lhrs, produced brownish and crisp powders due to condensation reaction on decomposition, dehydration and formation of sol-gel. Hence, when the powder pre-heated at about $100^{\circ}C$ was then heated at $1200^{\circ}C$ for 3hrs in atmosphere, the luminescence properties of resultant $Gd_{2}O_{3}:Eu^{3+}$ phosphor was measured by SEM, FT-IT and brightness intensity was shown 20% higher than those prepared by conventional method and by other chelating agent.

키워드